Article
How pH Windows and SX Stages Achieve 99.8% Nickel Purity
Industry: Nickel_Mining | Process: Refining
Refining nickel from acidic leach liquors is not alchemy. It is exact science. Start at pH ≈1–2. Oxidize ferrous iron (Fe²⁺) to ferric (Fe³⁺). Then raise the pH in tight steps. Impurities fall out while nickel and cobalt stay put. In practice, that means nearly 100% iron removal at pH 2.5–3.3 with only ~1–1.8% nickel/cobalt loss. Residual Fe drops to ~2 mg/L after a second neutralization. Temperatures are held at ~90–95 °C to keep solids filterable (researchgate.net).
With copper, the window shifts. Hydroxide precipitation clears Cu at around pH 7, but Ni barely moves until ≈10. Copper can also be sulfided as CuS at pH ~2 because its solubility product is very low (Ksp ∼10^–45 vs. NiS at ∼10^–20) (researchgate.net). The result is a clean Ni/Co sulfate liquor ready for solvent extraction.
Iron removal by controlled pH
Process engineers begin with oxidants such as H₂O₂ or air to convert Fe²⁺ to Fe³⁺, then add base. One study (Silva et al.) raised an iron‑rich laterite pregnant leach solution (PLS, leach liquor) from pH ~1.6 to 2.5–3.3 using NH₄OH (ammonium hydroxide). At pH 2.5–3.3, nearly 100% of dissolved iron precipitated, mainly as jarosite/goethite (iron sulfate and iron oxyhydroxide solids). Ni²⁺ and Co²⁺ losses were only ~1–1.8% (researchgate.net).
The precipitate (mixed K/NH₄ jarosite and goethite) settled well. A second neutralization with lime (CaO) to pH ~3.7–3.8 then pushed residual Fe down to ~2 mg/L, mostly as bassanite/gypsum. Ni/Co losses were still <1.6% (researchgate.net). The two‑stage scheme (ammonia then lime) removed >99% of iron and kept >98% of Ni/Co. Precipitation temperature was kept high (~90–95 °C) to improve filterability (same source). Base addition needs tight control at these narrow pH setpoints. Therefore plants use accurate chemical metering equipment such as a dosing pump to follow the pH rise closely without overshoot.
When solids settle well, facilities usually move to solid–liquid separation. A clarifier gives a defined detention time to remove suspended precipitates before the downstream circuits.
Copper out at pH 7, nickel stays soluble
Copper behaves differently from nickel. Its hydroxide solubility is much lower. One study neutralized a Cu–Ni wastewater and found Cu²⁺ precipitating almost completely by pH ≈7, but Ni²⁺ only began to precipitate at ≈10 (researchgate.net). In practice, Ca(OH)₂ addition to ∼pH 7 can remove ~100% of copper as Cu(OH)₂ with negligible nickel loss, because Ni ≫ Cu solubility (same source). Conversely, Ni²⁺ needs pH ~9–10 to co‑precipitate. Therefore it stays in solution at pH 7 (same source).
Hydrometallurgical nickel refining also uses selective sulfide precipitation. Adding a sulfide (for example Na₂S/H₂S) at pH ~2 removes copper as CuS (Ksp ∼10^–45) while nickel remains soluble (NiS Ksp ∼10^–20) (researchgate.net). Where settling rates need a boost in these steps, operators usually dose polymers. A targeted flocculant increases particle agglomeration and improves separator efficiency without changing the underlying pH chemistry described in the studies.
Stepwise neutralization results
Key outcome across the iron and copper stages: stepwise neutralization drops out the targeted impurities. Typical results are >99% Fe removal (for example to <2 mg/L) with <2% Ni/Co carry‑loss (researchgate.net). If copper is present, it is removed at a higher pH (hydroxide or sulfide precipitation) long before appreciable nickel hydroxide forms (researchgate.net). This leaves a purified Ni/Co sulfate liquor to feed the SX circuit.
Multi‑stage solvent extraction (SX) circuits
After impurity precipitation, Ni²⁺ and Co²⁺ remain together in the sulfate liquor. Commercial refiners use multi‑stage counter‑current SX (solvent extraction, a liquid–liquid separation) to split them. Two general schemes are standard: (a) Ni‑first circuits that extract nickel into the organic phase then strip it off (producing Ni electrolytes for electrowinning, EW), and (b) Co‑first circuits that selectively extract cobalt, leaving nickel in the raffinate. Both routes achieve very high purities and recoveries when staged in counter‑current.
One charts‑based nickel‑extraction flow (Bulong, Western Australia, 1999–2003) used direct SX on dilute leach liquor (no intermediate cake). The circuit produced a concentrated NiSO₄ strip liquor that yielded >99.8%‑pure Ni cathode on EW. Overall nickel recovery from PLS to Ni product was ≈98.2%, and cobalt recovery to a separate Co‑rich strip liquor was ≈98.5% (researchgate.net). In operational terms, typical aqueous Ni breakthrough was ~1–2%, and Co breakthrough ~1–2%, which shows tight separation (same source).
Co‑selective extraction using Cyanex 272
Another route starts with an extractant that selects cobalt. Cyanex 272 (a phosphinic acid) is known for its Co/Ni selectivity. At one pH charge (∼7.2), a Nordhoff separation factor of ~8000 for cobalt over nickel was reported (researchgate.net). Kasese Cobalt Ltd. (Uganda) and others built on this. An SX train with Cyanex 272 extracted Co²⁺ (and Mn²⁺) and left Ni²⁺ in the raffinate. Any trace nickel co‑extracted was scrubbed out via a CoSO₄ wash (researchgate.net). Subsequent stripping gave a pure cobalt liquor and a nickel‑rich raffinate. A follow‑up 3‑stage D2EHPA extraction then separated Mn²⁺ from Co²⁺. This gave final raffinate streams of ~99.9%‑pure Co, Mn, and Ni (same source). In short, consecutive SX (Cyanex 272 step + D2EHPA step) delivered essentially 100% pure Ni²⁺ and Co²⁺ products (same source).
D2EHPA, Versatic/LIX, and selective stripping

Other circuits use D2EHPA (di‑(2‑ethylhexyl) phosphoric acid) or Versatic 10/LIX systems. In these systems Ni and Co co‑extract at first, usually at pH ~3–5. Then staged stripping splits them. In an ammoniacal LIX example for Ni & Cu SX, >99% nickel extraction was achieved in 3 stages. Then >99.9% nickel strip in five stages (redesign.911metallurgist.com). In a strong acid/sulfate system, a multi‑stage counter‑current SX with 1 M D2EHPA can extract essentially all Ni and Co. Conventional strip stages, first Ni then Co, yield separate high‑purity products. In practice, design data confirm the approach. Ni recoveries to final Zn‑free Ni electrolyte routinely exceed 98%, and Co recoveries exceed 98%. Product purities are ≥99%. For example, Ni cathode is >99.8% Ni and theoretical Ni electrolyte is >99.9% pure (researchgate.net; researchgate.net).
In these SX schemes, pH control is important. If the pH is too high, impurities co-precipitate or co-extract. If it is too low, the target metals are left behind. Extractant dosing in cascaded stages usually runs 1–20 vol% organics. The dose is adjusted to meet the breakthrough and strip targets in the plant and bench data. The flows mention ammonia (NH₄OH) for jarosite-mode iron removal, lime (CaO) for final clean-up, and sodium sulfide for CuS precipitation. These are part of standard hydromet circuits. A supplier with a complete range of water and wastewater chemicals helps align availability to the pH windows cited. The process targets clean-metals performance that fits downstream electrowinning or saleable sulfate products. It also runs under regulatory constraints (for example, Indonesian discharge pH 6–9).
Figures and metrics recap
-
99% Fe removal (e.g., to <2 mg/L) at pH 2.5–3.3 (researchgate.net)
- <2% Ni/Co loss during Fe precipitation (researchgate.net)
-
98% Ni recovery (to Ni product) and >98% Co recovery in SX (researchgate.net)
- Ni strip yields at 99.9% of loaded Ni in multi‑stage SX (redesign.911metallurgist.com)
- Ni cathode purity >99.8% and Co/Mn stream purity >99.9% (researchgate.net; researchgate.net)
All of this depends on getting the chemistry right as documented. Oxidize Fe²⁺. Track pH precisely through 2.5–3.3 and ~3.7–3.8. Keep precipitation hot (~90–95 °C). Clear copper around pH 7 or via sulfide at pH ~2. Run multi-stage SX with disciplined pH and organic loading. Operations need supporting equipment around these steps, from accurate metering to solid–liquid separation. These choices slot in behind the chemistry rather than define it.
Sources for the figures and flows discussed include peer‑reviewed studies and industry reports: researchgate.net, researchgate.net, researchgate.net, researchgate.net, researchgate.net, and redesign.911metallurgist.com.