WhatsApp

Article

Inside the cold mill’s clean room: how alkaline and electrolytic stages strip rolling oils at 600 m/min

beta-pramesti-asiaindustry-steel-manufacturingprocess-hot-dan-cold-rolling

Inside the cold mill’s clean room: how alkaline and electrolytic stages strip rolling oils at 600 m/min

Cold-rolled strip leaves the mill wearing a film of oil and fines. High-throughput lines answer with [caustic chemistry, electric bubbles, and vigilant bath housekeeping](https://beta.co.id/en/blog/how-cold-mills-strip-oil-fast-inside-alkaline-baths-electric-bubbles-and-the-fight-to). The degreasing is fast and consistent. That is what makes annealing, coating and plating quality possible.

Industry: Steel_Manufacturing | Process: Hot_&_Cold_Rolling

Cold-rolled steel comes out of reduction with a thin film of rolling lubricants and fine metal particles on it. This film must be removed before annealing, coating or plating downstream. If it stays, it causes defects and poor adhesion (chemical.kao.com) (www.scribd.com).

Modern cleaning and degreasing lines combine mechanical and chemical stages. One industry supplier lists high‑pressure hot‑water wash, [neutral‑detergent wash with brushes](https://beta.co.id/en/blog/neutral-washes-oil-films-and-a-data-driven-plan-the-chemical-program-extending-harvester-life), alkaline degreasing baths, acid pickles, electrolytic degreasers, or combinations of these (www.salico.net). SALICO cites lines that handle strip up to 6.5 mm thick and 2.5 m wide, at speeds up to ~600 m/min (www.salico.net). Therefore each stage must act quickly.

Alkaline degreasing bath parameters

Alkaline degreasing uses caustic detergents such as NaOH or KOH plus surfactants at high pH (usually pH 12–13). It is the workhorse for heavy rolling oil removal. Immersion baths usually run 3–10% alkali and 50–95 °C with 3–10 minutes dwell. Sprays at 1.4–2.0 bar and 50–65 °C can clean in ~3 minutes (www.solverchem.com) (www.solverchem.com). The bath saponifies and emulsifies the oil (saponify: convert oils to soap‑like, water‑dispersible compounds). Formulations usually include wetting agents or chelants to lift iron fines. Alkaline detergents remove both the rolling oil film and fine iron particles embedded in the strip (chemical.kao.com).

Effectiveness depends on tight control of pH, alkalinity and temperature, and on equipment upkeep. Pumps, spray bars and filters must be designed for frequent maintenance (www.salico.net). Without upkeep, baths quickly saturate with oil and dirt and lose strength. A bath usually lasts about 1–2 weeks before it needs replacement or rejuvenation (chempedia.info).

To extend bath life, mills use continuous filtration or oil–water separation. Microfiltration (0.2 μm) at 40–70 °C is reported at ~250 L/m²·h. It can keep oil in the treated water below ~100 ppm. This extends bath life by about 5×, with payback within ~2 years (chempedia.info) (chempedia.info). In routine operation, baths are kept in continuous recirculation and floating oil is skimmed. Periodic filter changes prevent particulate build‑up. SALICO stresses pump/filter access and quick‑change elements to keep contamination in check (www.salico.net).

Operating ranges at a glance

  • Concentration: ~3–10% NaOH or equivalent (www.solverchem.com).
  • Temperature: 50–95 °C (usually ~60 °C) (www.solverchem.com).
  • Time: 3–10 minutes immersion. Sprays take ~3 minutes at 50–65 °C (www.solverchem.com).
  • Bath life: ~1–2 weeks before saturation. With microfiltration it lasts ~5× longer (chempedia.info) (chempedia.info).
  • Oil removal: usually more than 95% of residual oil is emulsified or saponified in a dedicated pass.

Electrolytic alkaline cleaning (HCD)

Thin or stubborn oil films need more. For these, mills add electrolytic cleaning. The strip passes through an alkaline electrolyte under DC current (direct current). Hydrogen and oxygen form at the surface and the bubbles scrub away contamination. Many lines run HCD (high‑current‑density) cleaning, usually 5–15 A/dm² (amps per square decimeter). Aluminum or stainless electrodes make the bubbles. China Steel Corporation describes an HCD line with an alkaline cleaning tank, a brush tank and a rinse tank to remove attached rolling oil (www.csc.com.tw) (www.scribd.com).

Vendors emphasize speed and thoroughness. They say electrolytic cleaning gives a totally clean surface and works better than conventional spray or immersion washes (www.scribd.com). It runs at line speed. SALICO cites up to ~600 m/min for cleaning lines (www.salico.net). The electrolytes usually contain NaOH (~1–4%) and anticorrosion additives. Mills may put a light alkali pre‑wash (NaOH ~1–3%) before the electrolytic tank (patents.google.com). Together they remove >99% of oil in one pass. The surface is then ready for annealing or coating.

Electrolytic cleaning also changes the waste profile. It does not use strong chemical detergents or solvents, so it can reduce chemical costs and waste. The oily effluent is mostly dilute alkali plus emulsified oil, and oil–water separators can treat it. Some systems are designed to recycle their electrolyte. Market adoption shows what OEMs demand for clean surfaces. An industry report notes a substantial global market for steel electrolytic degreasing chemicals, with ~38% of demand from auto manufacturers in 2023 (pmarketresearch.com).

Bath cleanliness and monitoring routines

Both alkaline and electrolytic stages need clean, well‑controlled baths. SALICO emphasizes routine swaps of squeegee rolls, spray bars, brushes, and backup rolls, and ready access to pumps, filters, and sensors (pH, conductivity, temperature) for easy servicing (www.salico.net). Sensors usually monitor bath pH and conductivity continuously. Therefore operators can add reagents or replace the bath when needed. Changing filters regularly (or backwashing) removes dispersed particles and emulsified oil. Floating skimmers capture free oil.

Once degreasing baths become “polluted” with oil they must be changed, usually within a few weeks, if not supported by filtration (chempedia.info). With continuous microfiltration holding oil below ~100 ppm, bath life extends by ~5× (chempedia.info). The economic impact is tangible. Cleaner, well-maintained baths mean consistent oil removal, fewer rejects, and lower chemical consumption over time.

Environmental compliance is part of the calculation. In Indonesia, spent rolling oils and emulsions are classified as hazardous B3 waste and need special handling (www.researchgate.net). Discharge limits for metal finishing streams can be tight. Oil and grease is limited to 5.0 mg/L for plating effluent (www.scribd.com). Therefore it matters that the oil is captured inside the plant. In practice, mills recycle rinse water and use skimmers or coalescers so the effluent complies. Electrolytic stages paired with oil–water separation keep the loads in check (www.salico.net) (chempedia.info).

Line configurations and throughput

Suppliers list the steps that go with each other: High‑Pressure Hot Water (HPHW) to blast off loose oil, neutral cleaning with mild detergents and brushes, alkaline degreasing, acid cleaning to remove scale, and electrolytic degreasing (www.salico.net). The exact configuration depends on the incoming oil and fines and on the target cleanliness. However, the speed is the same on every line. Lines process 6.5 mm‑thick, 2.5 m‑wide strip at up to ~600 m/min and still keep the cleaning performance (www.salico.net).