A corrosion coupon measures average mass loss and the form of attack on a specific material during exposure. Results are comparable only when alloy, preparation, area, rack position, flow, temperature, duration, cleaning and calculation stay consistent. Coupons do not reproduce heat transfer at condenser tubes. Therefore interpret them with water chemistry, chemical residuals, deposits, leakage, inspection and operating data.

Last technically reviewed: 1 August 2026.

Standards that control coupon testing

ASTM D2688-23 is the most direct reference for water systems. It determines corrosion rate by coupon weight loss and evaluates pitting in a side-stream rack. Its stated applications include open recirculating cooling water, closed chilled water and hydronic heating. However, the method operates without heat transfer.

ASTM G1-25 covers specimen preparation, removal of corrosion products and evaluation. Its cleaning procedures aim to remove corrosion products without significant base-metal loss. Over-cleaning inflates the apparent corrosion rate. Use the standard edition named in the company procedure and document any alternative method.

DocumentQuestion answeredInterpretation boundary
ASTM D2688-23How to expose coupons in a side-stream water system and determine weight-loss corrosion rate/pittingDoes not reproduce heat flux, boiling, real equipment crevices, galvanic couples, or dead zones
ASTM G1-25How to prepare, clean, and evaluate a specimen without excessive base-metal lossCleaning must suit the alloy and be recorded; results from different methods are not automatically comparable
Site and OEM procedureAlloy, rack point, flow, exposure period, control limit, response, and facility safetyMust not conflict with the contract standard, equipment metallurgy, or HSE approval

Do not claim “ASTM compliant” when a laboratory only weighs the coupon. The laboratory also needs area, density, exposure time, cleaning blank/control and water-condition records. The audit trail is part of the result.

Place the corrosion rack where it represents the system

The rack must receive continuously representative loop water. It must not sit in stagnant water in a dead leg, and it must not get flow only when an operator opens a valve. Identify the location on the P&ID. Provide safe isolation/depressurization, a flow indicator or verification method, and a drain routed into the site’s treatment system.

Placement checkRecord requiredRisk if wrong
Side-stream sourceSupply/return point and relation to exchangers, basin, pump, filter, blowdown, and chemical injectionSample does not represent the loop or sees only a chemical slug
Rack flowValue/range, measurement method, valve position, operating hours, interruptionLow flow creates deposits/stagnation; changed flow invalidates trend comparison
TemperatureMinimum, normal, maximum, and seasonal/load changesReaction and deposits change; a cold rack does not represent a hot surface
Injection pointDistance and mixing after inhibitor, acid, and oxidizing/non-oxidizing biocideLocal concentration may attack the coupon or give an optimistic result
Coupon materialAlloy/grade representing carbon steel, copper alloy, stainless, galvanized, or another site materialA generic coupon does not answer the actual material risk
Coupon arrangementPosition, orientation, insulator, fastener, and order per the approved methodGalvanic contact, copper deposition, shielding, or an artificial crevice
Safe accessIsolation, pressure relief, labels, PPE, sampling, drain, and lockoutHot/chemical exposure and loss of coupon/data

Place the rack after complete chemical mixing when monitoring treatment performance. However, avoid a point that only sees a transient high concentration near an injection quill. If supply/return or another risk area needs comparison, use separately identified racks or monitors. Do not move one rack and merge two baselines.

Record sheet for every coupon

Capture data before insertion, through exposure and at removal. Photograph the as-received coupon, the removed coupon before cleaning, and the cleaned coupon with a scale and visible coupon ID.

  1. Coupon ID, alloy/grade, heat/lot where available, density used, dimensions, exposed area, hole/edge treatment, initial mass, and balance.
  2. Installation/removal date and time, exposure hours, shutdown, flow interruption, draining, layup, and tower cleaning during the interval.
  3. Rack location on the P&ID, slot, orientation, fastener/insulator, flow, pressure, and temperature range.
  4. Makeup and circulating-water chemistry: pH, conductivity, cycles, hardness, alkalinity, chloride, sulfate, silica, iron, copper, turbidity/TSS, and the site’s microbiological parameter.
  5. Treatment: product, target and measured residual, dose, pump calibration, injection point, blowdown, acid feed, biocide event, and deviation.
  6. Final mass after cleaning, cleaning method and blank/control correction where needed, visual morphology, pit data, deposit analysis, and reviewer.

Betaqua Sentinel CTS cooling-tower monitoring can help record operating parameters continuously. Coupons give material evidence. Sensors and water analysis explain what happened between insertion and removal.

Qualify the result before changing the inhibitor programme

Assign every result a usable, qualified, or invalid status before it enters the trend. Usable means the method and exposure match the comparison basis. Qualified means the value can be reported with a deviation that limits interpretation. Invalid means method error cannot be separated from mass loss or exposure condition. Decide the status before you see whether the number looks “good” or “bad.”

Data conditionInitial statusTreatment
ID, alloy, area, density, time, flow, cleaning, and mass balance are completeUsable when all meet the procedureTrend with chemistry, residual, events, photographs, and pit data
Shutdown/flow interruption is recorded, while identification and handling remain correctQualifiedReport duration and condition; do not compare directly with normal exposure without the qualification
Rack flow is unknown or the coupon was dry/stagnant for an unknown periodInvalid for the normal trendInvestigate the rack, install a new coupon, and retain the old value only as a deviation record
Cleaning blank/control shows base-metal loss material to coupon mass lossQualified or invalid under the procedureApply only the correction allowed by the method; repeat when correction is not defensible
Coupon ID/alloy is mixed up, area/density cannot be proven, or final mass is not traceableInvalidDo not calculate a rate; repeat with complete chain of custody
Average rate is low while a significant pit, crevice, or local deposit is presentUsable for general corrosion, qualified for integrity conclusionsEscalate localized-attack inspection; never clear the equipment on average rate alone

Check repeatability with parallel coupons

Parallel coupons of the same alloy, lot, position, flow, and interval help expose variation in the rack, preparation, cleaning, or weighing. Calculate relative percent difference (RPD) = |A − B| ÷ ((A + B) ÷ 2) × 100%. If two example results are 0.020 and 0.024 mm/year, their RPD is 0.004 ÷ 0.022 × 100% = 18.2%.

This page does not impose a universal RPD limit. The laboratory or site should predefine its acceptance criterion from the method, alloy, expected mass loss, balance capability, and historical baseline. If RPD fails, do not average the values to hide the disagreement. Check slot position, flow, handling, cleaning blank, balance resolution, deposit, and the morphology of each coupon.

Consider a change to the cooling-tower corrosion inhibitor only after the result passes qualification and is correlated with chemistry, residual, blowdown, load, and equipment inspection. One invalid result is a data-quality problem. It is not evidence that the dose should rise.

Corrosion-rate formula and worked example

A common metric weight-loss calculation is:

CR (mm/year) = 87.6 × W ÷ (D × A × T)

Here W is mass loss in mg, D is alloy density in g/cm³, A is exposed area in cm², and T is exposure time in hours. The area must follow the approved method. Mass loss must be corrected for the applicable cleaning procedure.

Transparent worked example

A carbon-steel coupon has density 7.86 g/cm³, exposed area 28.0 cm², exposure 720 h, initial mass 32,415.0 mg, and cleaned final mass 32,375.0 mg. Its mass loss W is 40.0 mg.

CR = 87.6 × 40.0 ÷ (7.86 × 28.0 × 720) = 0.022 mm/year.

That is about 0.87 mil per year (mpy) because 1 mpy equals 0.0254 mm/year. Keep the unrounded calculation. Recalculate whenever area, time, density, or cleaning correction changes. Never copy a constant without checking its units.

Interpret the number without losing context

ASTM D2688-23 describes results as relative. Compare one material with the same material in another water condition, or compare inhibitor performance with a controlled baseline. Therefore a universal limit for every cooling tower is not defensible.

FindingSupported conclusionNot yet proven
Mass-loss rate falls for the same alloy, rack, and intervalAverage general corrosion improved under that exposureEvery exchanger/tube is safe or localized corrosion is absent
Low weight loss with a deep/local pitGeneral corrosion is low, but localized attack may be significantAverage rate is adequate as the only KPI
Thick coupon depositDeposit loading/fouling occurred at the rackDeposit composition or cause without analysis
One high interval during loss of rack flowStagnation affected the result, so it is not directly comparable to the normal-flow baselineThe whole loop experienced the same rate
Copper/alloy result changes with dissolved iron/copperA change needs correlation with water chemistry and metallurgyThe corrosion source location without further inspection/trending

At minimum report average corrosion rate, before/after-cleaning photographs, attack morphology, pits/crevices, deposits, and exposure deviations. Heat exchangers with heat flux, crevices, stress, deposits, high velocity, or mixed metallurgy still need inspection/NDT under the mechanical-integrity program.

Inspection and coupon-replacement cadence

Use the fixed exposure period in the site or contractual procedure based on ASTM D2688-23. Compare intervals only when material, rack, flow, and duration remain consistent. Pulling the only coupon early “for a quick look” gives a non-comparable result dominated by initial surface conditioning.

  • At commissioning or a program change: install new coupons after rack flow, water chemistry and dosing are stable. Freeze the baseline before another change.
  • Each operator round: check for leakage, pressure, flow indication, valve position and air lock. Also check that the rack stays full. Do not remove coupons for a visual check.
  • At the site/laboratory interval: record chemistry and residuals with timestamps that map to the exposure.
  • At the fixed endpoint: remove, photograph, identify, seal/transport, clean, weigh, evaluate pits, and install a new coupon in the same position.
  • After a major upset: keep the running coupon and mark the event. If you need short-term evidence, add a separately identified parallel coupon. Do not break the primary series.

Review the frequency after a change of makeup source, higher cycles, a change of inhibitor or biocide, tower cleaning, an exchanger leak, process contamination, a side-stream filtration failure, or system layup and startup.

Response checklist when results deteriorate

Do not raise the inhibitor dose straight away. First prove the result is valid and find out what changed during exposure.

SignalFirst 24-hour checksNext action
Corrosion rate rises while chemistry looks normalCoupon ID/alloy/area/time, cleaning, balance, rack flow, shutdown historyRepeat with a controlled coupon if data are defective; inspect equipment if valid
pH falls or acid is overfedAnalyzer calibration, grab sample, dosing pump, valve/interlock, injection mixingStop/isolate overfeed per SOP, restore the envelope, inspect for localized damage
Conductivity/chloride/cycles riseBlowdown valve, conductivity controller, makeup, evaporation/load, leakRestore blowdown and cycle target; evaluate chloride/material limit
Inhibitor residual is lowTank level, solution strength, pump calibration, quill/check valve, flow-paced signalRestore measured dose and find the cause; do not raise stroke without calibration
Biofilm/deposit appearsBiocide residual/contact, microbial data, nutrients, side-stream filter, dead legsCoordinate cooling-tower biocides, cleaning, and deposit removal with corrosion control
Iron/copper or turbidity rises after an upsetProcess leak, makeup quality, transported corrosion products, tower cleaningIsolate the source, sample deposits, and inspect the relevant exchanger/piping

Coordinate cooling-tower corrosion inhibitors, scale inhibitors, biocide, blowdown, and filtration. Where chemical delivery is unstable, Watermart’s water-treatment dosing pumps are a relevant equipment handoff.

Data package for cooling-water program review

Provide the P&ID and water balance. Provide the tower volume and the circulation, makeup and blowdown flow. Provide the metallurgy for every exchanger and pipe circuit. Provide dated makeup and circulating chemistry, temperature and load, and the cycle target. Provide all chemicals, residuals, doses and pump calibration. Provide the rack drawing and flow. Provide coupon certificates, raw weights, area, density, exposure log, cleaning method, photographs and pit data. Provide the corrosion, scale and biofilm inspection, process leaks and maintenance history.

Laboratory cleaning chemicals, deposits and rack drain water belong in the site’s waste procedure. Indonesia’s Government Regulation No. 22 of 2021 covers water-quality protection and waste management. The waste classification and disposal must follow the actual composition and the facility’s environmental approval.