WhatsApp

Article

Inside the Dip: Why Bare Spots, Thick Coats, and Peeling Still Plague Hot‑Dip Galvanizing

beta-pramesti-asiaindustry-galvanizing-and-electroplatingprocess-galvanizing-hot

Inside the Dip: Why Bare Spots, Thick Coats, and Peeling Still Plague Hot‑Dip Galvanizing

ISO 1461 does not reject bare spots of 2–5 mm. However, brittle 200‑micron layers that flake are a different problem. The most expensive hot‑dip galvanizing defects usually start in pre‑treatment and get worse in the kettle. The fixes are documented: clean steel, controlled flux, 450–460°C zinc, and tightly timed immersions under ASTM A123/SNI 07‑7033 and ISO 1461.

Industry: Galvanizing_and_Electroplating | Process: Galvanizing_(Hot

In galvanizing, the smallest misses can grow into costly rework. Industry data note that repair of severe bare areas can increase project costs by 10–30%. Standards such as ISO 1461 allow only very limited bare spots (ckit.co.za). The root causes are usually in cleaning, pickling and fluxing. They are well known and measurable, and so are the process setpoints in the zinc bath.

The American Galvanizers Association and other guides make the same point in plain terms. Steel will not react with zinc to form a coating unless the surface is completely clean (agindo.org). ASTM A123 (widely referenced in Indonesian SNI 07‑7033) and ISO 1461 then set the acceptance bands for coating thickness and surface condition (bondigalva.co.id).

Bare spots: pre‑treatment and bath chemistry

Small uncoated areas are usually only a few millimeters across. They almost always come from surface prep or process errors. ISO 1461 explicitly excludes tiny bare spots (≈2–5 mm) from rejection. The standard notes that sacrificial zinc nearby still protects such minor areas (ckit.co.za). Root causes include leftover weld spatter, embedded debris or rust from incomplete cleaning, and coatings blocked by lifting wires or mill scale (studylib.net) (ckit.co.za).

Residual oil, grease or oxide films left by degreasing and pickling stop the zinc from bonding (agindo.org) (studylib.net). The flux layer is a zinc chloride–ammonium chloride salt film. It keeps fresh oxide off the steel before dipping. If this layer dries out, its iron phosphate film breaks down. This is called “over‑drying”. It happens when there are long delays or the part overheats before the dip. Then rust can form and the coating does not take (ckit.co.za). In the bath itself, too much aluminum, above ~0.007%, produces “black spots”, which are bare areas (ckit.co.za). Physical barriers also leave local bare patches. Examples are hooks, chains or sand trapped in castings (studylib.net) (fabmann.com).

In practice, the remedies are thorough cleaning and complete pickling. Clean with SP1 solvent degreasing, then rinse fully, so no mill scale remains. The flux needs to be fresh and in range, 2–4% ammonium chloride, and not over‑dried. Heat it and transfer the part to the zinc promptly, so the flux film stays active (ckit.co.za) (studylib.net). Design the hanging points to avoid contact marks. Very small spots (<~5 mm) are usually benign. Larger discontinuities need strip and re‑galvanizing (ckit.co.za) (studylib.net). Accurate chemical dosing helps control the flux (see dosing pumps). Standard plant utilities make complete rinsing easier (see supporting equipment for water treatment).

Excessive thickness: steel chemistry and time‑temperature

The target zinc thickness depends on the steel thickness. ASTM A123 Table 1, for example, needs 45–100 µm depending on the category (bondigalva.co.id). Coatings hundreds of microns thick usually point to material and process issues. Silicon and phosphorus in the steel act as catalysts for rapid Zn–Fe alloy growth. Steels with ~0.04–0.15% or >0.22% Si (the “Sandelin range”) and P>0.04% form unusually thick, matte coatings (fabmann.com) (azom.com).

Longer immersion times or higher bath temperatures also make the coating thicker. Batch loads usually soak for 3–10 minutes, and heavy loads soak longer. Therefore over‑immersion or “over‑soaking” gives a thicker coating than intended (azom.com). Poor drainage leaves zinc build‑ups, especially from deep holes or tight threads. The same happens if the excess zinc is not removed with an air knife. Very thick alloy layers (≈≥200 µm) become brittle and can delaminate from the steel (azom.com).

There are several controls. Choose steel chemistries with Si and P in the recommended bands (fabmann.com). Keep the dip timing precise. Use high‑pressure air knives or centrifuges on threaded parts. Check the coating weight against the ASTM tables (as adopted in SNI 07‑7033) to confirm the minimum µm for the steel gauge. For example, 6–13 mm plate must get ≥85–100 µm zinc. Much more than this gives little benefit and risks flaking (bondigalva.co.id) (azom.com).

Adhesion failures: brittle alloys and contamination

True adhesion failure, where the coating peels or flakes, is rare because zinc metallurgically fuses to steel. Failures usually involve special conditions. Thick‑coating scenarios on high‑Si/P steels produce brittle alloy layers. These layers crack and separate under thermal or mechanical stress (azom.com) (fabmann.com). Excessive cooling stresses can also cause interface cracks, for example when very thick, rigid coatings are quenched (azom.com).

Contamination matters too. Passivated surfaces prevent bonding. Chromate coatings are sometimes used in quench tanks to protect against “wet storage stain”, and they must be stripped before galvanizing (kta.com). Any oil or wax film left from fabrication can cause lifting. Neutral process controls include solvent degreasing and a check for residual chromate, for example the CuSO₄ test per SSPC‑SP16 (kta.com). Quenching practice also counts. A mild alkali quench, rather than plain water spray, minimizes thermal shock. If peeling is observed, it usually points to hydrogen embrittlement or a steel defect. Therefore the steel grade and the handling need investigation. Very thick coatings (>0.2 mm) are avoided because they are prone to spalling (azom.com).

Pre‑treatment controls: cleaning, pickling, fluxing

Cleaning and degreasing remove grease, oil and wax that block zinc bonding. Guides emphasize that steel will not react with zinc to form a coating unless the surface is completely clean (agindo.org) (studylib.net). Pickling (acid cleaning with HCl/H₂SO₄) removes rust and mill scale. Under‑pickling leaves scale or nitride films that cause localized bare spots. Over‑pickling carries a risk ("acid burn"), and prompt water rinsing mitigates it.

Fluxing (zinc chloride–ammonium chloride) lays down a thin salt film to prevent oxide before dipping. A concentration that is too low, aged flux, or parts that dry after fluxing (over‑drying) lead to bare spots. However, excess flux residue can be trapped as flux inclusions, a rare cause of white rust (ckit.co.za). [Holding flux at 2–4% ammonium chloride](https://beta.co.id/en/blog/galvanizers-are-stopping-the-drain-inside-the-chemistry-extending-flux-bath-life) and avoiding over‑drying are the main controls. Many shops do this with chemical dosing control (see dosing pumps) and by standardizing rinse utilities (see supporting equipment for water treatment).

Process setpoints: bath and time

Bath temperature and immersion time steer both thickness and adhesion. AGI notes the zinc kettle should run ~450–460°C for normal reaction (agindo.org). If bath aluminum or other additives drift out of range, defect rates climb. Immersion time should match load weight. Short dips yield thin spots. Over‑dipping yields excessive alloy and potential adhesion problems (azom.com) (azom.com).

Inspection, standards, and lifetime math

ASTM A123/SNI set minimum µm targets by steel gauge. A result outside the usual shop thresholds (±20–30%) means the part needs repair (bondigalva.co.id). Life expectancy is roughly linear with coating thickness. Going from ~50 µm to 150 µm can mean decades longer until the first maintenance (galvanizeit.org) (fabmann.com). Inspection based on data catches defects early. Check the coating thickness with gauges and look for gaps under 5 mm. Then you can plan rework or a design fix before a large failure (ckit.co.za).

Sources and cross‑references

Indonesian regulations (SNI 07‑7033) refer to ASTM A123/ISO 1461 norms (bondigalva.co.id). Industry guides (HDGASA, AGA) list the common defects and their causes (ckit.co.za) (studylib.net). Metallurgical studies and trade documents explain how steel chemistry affects the coating (fabmann.com) (azom.com). Galvanizing associations document the link between thickness and life (galvanizeit.org) (fabmann.com). The sources also list specific defect mechanisms: welding slag, sand inclusions and excess aluminum (studylib.net) (ckit.co.za). AGA and AGI also note setpoints such as the 450–460°C bath range and the need for perfectly clean steel (agindo.org). These sources back all the claims above.