WhatsApp

Article

Hospitals Are Winning on Legionella — and Losing Copper and Zinc

beta-pramesti-asiaindustry-hospital-industryprocess-legionella-control-dan

Hospitals Are Winning on Legionella — and Losing Copper and Zinc

Supplemental disinfectants control pathogens but they also speed up corrosion in copper and galvanized steel. New field data puts hard numbers on this tradeoff. It also shows why coupons, probes and tight chemistry control matter.

Industry: Hospital_Industry | Process: Legionella_Control_&_Prevention

Hospitals have used secondary disinfection to keep Legionella in check. However, the same chemicals that clean the water can quietly eat through the plumbing. In two Italian hospitals, corrosion coupons measured carbon-steel losses of ~0.11 mm/yr under monochloramine, ~0.14 mm/yr under chlorine dioxide, ~0.17 mm/yr under hydrogen peroxide, and ~0.14 mm/yr even when untreated (pmc.ncbi.nlm.nih.gov).

The morphologies differ. Chlorine dioxide produced uniform plus ulcerating corrosion. Hydrogen peroxide drove deep pitting. Monochloramine showed mostly uniform mild attack (pmc.ncbi.nlm.nih.gov, pmc.ncbi.nlm.nih.gov). Rates can stay “satisfactory” (below 0.25 mm/yr is usually treated as a maintenance threshold). However, the choice of disinfectant changes how and where metals fail. Therefore monitoring is important.

Chlorine residuals and copper loss

Chlorine (hypochlorite) is a strong oxidizer that speeds up copper corrosion. Field data show copper corrosion rates rise roughly in proportion to the residual dose (pmc.ncbi.nlm.nih.gov). In one study, copper coupons in tap water lost more mass as free Cl₂ increased from ~0.25 mg/L to 1 mg/L. Both the corrosion rate and copper leaching climbed in step (pmc.ncbi.nlm.nih.gov).

Even low‑level chlorination (~0.25–0.5 mg/L) caused a measurable copper loss of about 0.01 mg/d·cm² in lab tests (pmc.ncbi.nlm.nih.gov). Shock‑level treatments (5 mg/L) drove rates several times higher. In one immersion test they reached hundreds of mils per year (mpy, a corrosion unit) (pmc.ncbi.nlm.nih.gov). Galvanized steel (zinc‑coated) also suffers. Microscopy shows chlorine, and especially chlorine dioxide, dissolving zinc step by step. Copper surfaces turn porous as oxides form. This is classic dezincification on galvanized steel (pmc.ncbi.nlm.nih.gov).

Chlorine dioxide attack on copper and zinc

Chlorine dioxide (ClO₂) is strongly oxidizing and particularly aggressive to metals. At ~1 mg/L ClO₂ in lab simulations, copper converted to very porous copper oxide and galvanized steel showed intense dezincification (pmc.ncbi.nlm.nih.gov). Vertova et al. reported that ClO₂ makes copper surfaces “very porous” and strips zinc from galvanized steel (pmc.ncbi.nlm.nih.gov).

One accelerated study found “severe degradation” across copper and zinc materials under 0.8 mg/L ClO₂ at elevated temperature (pmc.ncbi.nlm.nih.gov). On carbon steel, hospital coupons under chlorite treatment measured ~0.14 mm/yr. That is close to the acceptable limits usually cited when the rate is written in hundreds of μm/yr (pmc.ncbi.nlm.nih.gov). The practical point: ClO₂ control needs rigorous coupon surveillance.

Monochloramine and the ammonia factor

Monochloramine (NH₂Cl) is a more stable biocide and oxidises less. Therefore it is usually less aggressive toward metals than chlorine or chlorine dioxide (www.sanipur.com). In Marchesi’s field work, carbon‑steel coupons under monochloramine averaged only 0.11 mm/yr. That was the smallest loss among the treatments (pmc.ncbi.nlm.nih.gov).

Monochloramine does not oxidize copper as readily as chlorine. However, its ammonia byproduct can cause localized pitting if nitrification takes hold. Plumbing programs therefore keep fresh hypochlorite and the right feed ratios to minimize ammonia spikes (pmc.ncbi.nlm.nih.gov). Chloramines still corrode copper and iron slowly, and they can cause biofilms if nitrification is not controlled (www.sanipur.com). Therefore even these systems need corrosion monitoring.

Hydrogen peroxide in complex formulations

Hydrogen peroxide (H₂O₂) is a strong oxidant and it can corrode copper badly. It is usually used in stabilized or “accelerated” blends. Nakhaie et al. reported that hospital‑grade accelerated H₂O₂ cleaners caused “considerably higher corrosion rates” on pure copper than H₂O₂ alone. This shows that routine peroxide disinfection readily dissolves copper (iopscience.iop.org).

In Marchesi's comparison, H₂O₂ treatment gave the highest steel coupon loss (~0.17 mm/yr) (pmc.ncbi.nlm.nih.gov). On galvanized steel, peroxide most likely oxidizes zinc quickly, and there are fewer specific data on this. Residuals above 10 mg/L need a close watch, because months of exposure can cause severe pitting and oxide formation.

Other disinfection modalities

Ozone and UV have little effect on the pipeline. Ozone does not keep a lasting residual deep in the system, and UV systems add no chemicals. [Copper–silver ionization (Cu–Ag)](https://beta.co.id/en/blog/hospitals-legionella-playbook-chlorine-dioxide-vs-coppersilver-vs-monochloramine) is not a “chemical” but a metal dose. It raises copper and silver levels. It can also cause galvanic corrosion of ferrous components if dissimilar metals touch (pmc.ncbi.nlm.nih.gov). Hospital cold and hot lines rarely use bare galvanized iron, so Cu–Ag is less common. If it is present, it makes steel parts rust faster (pmc.ncbi.nlm.nih.gov).

Corrosion monitoring: coupons and probes

When a chemical residual is present, routine corrosion monitoring is important. Place metallic coupons (strips of copper, galvanized steel, or stainless) in hazardous zones for 3–6 months, then measure the weight loss. This gives direct corrosion rates (mm/yr or mpy) (pmc.ncbi.nlm.nih.gov, pmc.ncbi.nlm.nih.gov). Marchesi’s 6‑month program returned 0.11–0.17 mm/yr losses (pmc.ncbi.nlm.nih.gov). Vertova et al. used scanning electron microscopy (SEM) to show oxide films and dezincified zones (pmc.ncbi.nlm.nih.gov).

Why it matters: chemical disinfection can push metal loss beyond design allowances. Without monitoring, pinholes or leaks may surface months or years later. Corrosion also consumes disinfectant, because free chlorine reacts with metal oxides. It also releases iron and copper that can feed biofilms (pmc.ncbi.nlm.nih.gov). Beyond coupons, facilities deploy corrosion probes for real-time indices, including anodic/cathodic half‑cell meters and linear polarization resistance (LPR) probes. Periodic sampling for dissolved Cu, Zn, and Fe and analyzing scale chemistry complements the picture. Tracking trends is the trigger: a rising copper concentration or increasing pitting coverage on removed coupons is a red alert.

Water safety plans (WSP) and engineering guidance (for example ASHRAE, AWWA) treat corrosion control as a parallel requirement. If a secondary disinfectant is added, its impact on materials should be tracked. Indonesian health guidance also emphasizes [Legionella risk management via a WSP](https://beta.co.id/en/blog/hospitals-are-turning-water-plans-into-hard-proof-heres-the-data-playbook-that-keeps) that includes water temperature and chemistry control (pmc.ncbi.nlm.nih.gov). The 2019 “Pedoman Pencegahan dan Pengendalian Legionellosis” focuses on pathogen control. However, its principles imply corrosion monitoring as part of managing hospital water distribution systems.

Water chemistry management parameters

Keeping pH and alkalinity in a good range keeps metals stable. Copper is most stable near neutral to slightly alkaline pH. Soft, acidic water (pH < 6.5) dissolves copper quickly (www.ncbi.nlm.nih.gov). WHO guidance notes that neutral to alkaline pH (7–9) and moderate hardness help form a protective copper carbonate film (www.ncbi.nlm.nih.gov). For galvanized/steel, the best pH is usually ~6.8–7.5, and one guideline recommends 6.8–7.3 for iron networks (www.ncbi.nlm.nih.gov).

Enough alkalinity (≥40 mg/L as CaCO₃) and a slightly positive Langelier Index (a measure of scaling tendency) promote protective calcium carbonate on steel. In practice, buffering with soda ash or lime and keeping alkalinity at ≥40–60 mg/L helps (www.ncbi.nlm.nih.gov). Where orthophosphate or silicate films are suitable, targeted dosing of a corrosion inhibitor can cut iron/copper release. WHO notes that orthophosphate is widely used to prevent "red water" from iron corrosion. The dose must be managed to avoid phosphate-induced biofouling (www.ncbi.nlm.nih.gov).

Chloride control matters. Chloride promotes copper pitting and galvanic action at soldered joints. Experience from lead/copper programs implies keeping the chloride‑to‑sulfate mass ratio (CSR) low. Guidance points to CSR < 0.5 to avoid pitting (www.researchgate.net). If the source water has high chloride (for example, sea salt intrusion), you need additional inhibitors or pH adjustments.

Disinfectant residuals should be optimized. Higher is not always better. Aim for the minimum effective residual, about 0.5–1.0 mg/L Cl₂ or 2–4 mg/L ClO₂ at outlets. This limits oxidant stress and still works. In Marchesi’s dataset, Legionella control was achieved at ~3 mg/L monochloramine. Therefore higher doses are not needed (pmc.ncbi.nlm.nih.gov). Frequent flushing reduces stagnation, which can locally spike oxidants. Measured chemical feed using dosing pumps helps keep these setpoints tighter.

Dissolved oxygen and temperature also influence rates. Aerobic conditions speed iron corrosion, so deaerated makeup and minimizing open storage can help. Keeping hot water in "Legionella‑safe" ranges (50–55 °C) reduces dissolved oxygen. Large temperature swings can stress protective films, so stable recirculation is preferred. Monitoring data should drive adjustments. For example, if coupons show rising copper loss, nudge pH upward or refine inhibitor dose. Where galvanic coupling is evident, change materials or introduce dielectric unions.

Program thresholds and response

A balanced hospital strategy accepts that chemical disinfection increases corrosion stress on copper and galvanized components. However, it uses monitoring and chemistry control to bound the risk. Acceptable coupon losses might be on the order of ~0.1–0.2 mm/yr. If surface loss exceeds ~0.25 mm/yr (≈250 μm/yr), act immediately. Switch the disinfectant or apply inhibitors (and, where appropriate, water conditioning). With careful control, facilities can get the antimicrobial benefits without unduly shortening plumbing life. These recommendations reflect peer‑reviewed studies and WHO/AWWA treatment guidance (pmc.ncbi.nlm.nih.gov, pmc.ncbi.nlm.nih.gov, iopscience.iop.org, pmc.ncbi.nlm.nih.gov, www.ncbi.nlm.nih.gov, www.ncbi.nlm.nih.gov).